为有效去除锌湿法冶金过程中的微量钻,探索采用臭氧氧化净化ZnSOt溶液中钴的可行性,考察搅拌速度、反应温度、气体流量、溶液pH值、钴离子浓度、锌离子浓度等因素对除钴效果的影响。结果表明:在锌离子初始浓度100g/L、钴离子初始浓度20mg/L、温度30℃、气体流量800mL/min、pH=5.0、搅拌速度800r/min等条件下,反应30min后,钴浓度可降至0.2mg/L,除钴率高达99%。
In order to remove trace cobalt in the process of zinc extractive hydrometallurgy, a novel method to precipitate cobalt from ZnSO4 solution by ozone oxidation was proposed. The factors influencing the effect of removing cobalt, including stirring speed, temperature, gas flow rate, pH and concentrations of cobalt ion and zinc ion were investigated. The results show that the cobalt concentrations and elimination rate can reach 0.2 mg/L and 99%, respectively, under the solution conditions as initial concentrations of cobalt and zinc 20 mg/L and 100 g/L, controlling pH of 5.0, stirring speed of 800 r/min, gas flow rate of 800 mL/min, reacting time of 30 min at 30 ℃.